欢迎访问《中外公路》官方网站,今天是
分享到:
二阶热固性环氧沥青桥面铺装黏层黏结性能试验研究
CSTR:
作者:
作者单位:

(1.宜昌市交通运输局 ,湖北 宜昌 443000 ;2.宜昌市城市建设投资开发有限公司 ,湖北 宜昌 443000 ;3.沈阳建筑大学 材料科学与工程学院 ,辽宁 沈阳 110168 ;4. 武汉理工大学 硅酸盐建筑材料国家重点实验室 ,湖北 武汉 430070 )

作者简介:

周昌栋,男,大学本科,教授级高级工程师.E-mail:1944635770@qq.com

通讯作者:

丁庆军,男,博士,教授,博士生导师.E-mail:dingqj@whut.edu.cn

中图分类号:

U443

基金项目:

国家自然科学基金资助项目(编号:U21A20149);硅酸盐建筑材料国家重点实验室开放基金资助项目(编号:SYSJJ2020-07);沈阳市中青年科技创新人才支持计划项目(编号:RC220313);辽宁省教育厅高校基本科研项目(编号:LJKMZ20220950)


Experimental Study on Adhesive Pe rformance of Second-Order Thermosetting Epoxy Asphalt in Bridge Deck Pavement
Author:
Affiliation:

(1.Yichang Transportation Authority , Yichang , Hubei 443000 , China ; 2. Yichang Urban Construction Investment and Development Co ., Ltd., Yichang , Hubei 443000 , China ; 3.School of Materials Science and Engineering , Shenyang Jianzhu University , Shenyang , Liaoning 110168 , China ; 4.State Key Laboratory of Silicate Materials for Architectures , Wuhan University of Technology , Wuhan , Hubei 430070 , China )

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    该文以宜昌伍家岗长江大桥为工程依托,针对铺装结构中 RA沥青混凝土与高黏高弹 SMA 沥青混凝土层间的二阶热固性环氧沥青材料的不同洒布量、不同第一阶段固化时间、不同养护时间、不同服役温度下的界面抗剪与拉拔强度以及洒布量对耐剪切疲劳性能的影响开展研究。研究结果表明:随着二阶热固性环氧沥青洒布量的增加,黏结与抗剪强度提高,结构耐剪切疲劳性能增强,施工环境温度为 25~35 ℃时,二阶热固性环氧沥青黏结层与高黏高弹 SMA的 施 工 间 隔 建 议 44~52 h,施 工 完 成 后 封 闭 养 护 时 间 应 大 于 7 d,二 阶 热 固 性 环 氧 沥 青 黏 层 可 实 现 组 合 铺 装 结 构 的25 ℃抗剪强度 ≥3.8 MPa,拉拔强度 ≥1.7 MPa,60 ℃抗剪强度 ≥1.7 MPa,拉拔强度 ≥0.9 MPa,研究结果对二阶热固性环氧沥青材料在桥面铺装工程中的应用具有指导意义。

    Abstract:

    Based on the Wujiagang Yangtze River bridge project in Yichang,the interfacial shear strength and pull-out strength of the second-order thermosetting epoxy asphalt material between RA asphalt concrete and high viscoelastic SMA asphalt concrete in pavement structure were studied under different spraying amount,different first-stage curing time,different curing time,and different service temperatures.In addition,the influence of spraying amount on shear fatigue resistance was studied.The results show that with the increase in the spraying amount of the second-order thermosetting epoxy asphalt,the adhesive performance and shear strength are improved,and the shear fatigue resistance of the structure is enhanced.At a construction ambient temperature of 25?35 ℃,the construction interval of second-order thermosetting epoxy asphalt layer and high viscoelastic SMA asphalt concrete is recommended to be 44?52 h.Closed curing time after construction should be more than 7 days.The second-order thermosetting epoxy asphalt layer can achieve the shear strength of ≥3.8 MPa and pull-out strength of ≥1.7 MPa of the composite pavement structure at 25 ℃,as well as shear strength of ≥1.7 MPa and pull-out strength of ≥0.9 MPa at 60 ℃.The research results have guiding significance for the application of second-order thermosetting epoxy asph alt material in bridge deck paving engineering.

    参考文献
    相似文献
    引证文献
引用本文

周昌栋,代明净,赵明宇,等.二阶热固性环氧沥青桥面铺装黏层黏结性能试验研究[J].中外公路,2024,44(3):129-136.
ZHOU Changdong, DAI Mingjing, ZHAO Mingyu, et al. Experimental Study on Adhesive Pe rformance of Second-Order Thermosetting Epoxy Asphalt in Bridge Deck Pavement[J].中外公路,2024,44(3):129-136.

复制
分享
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2022-11-24
  • 最后修改日期:
  • 录用日期:
  • 在线发布日期: 2024-06-27
  • 出版日期:
文章二维码
网站二维码
期刊公众号